Controlled thermal pre-treatment of ZMG232G10® for corrosion mitigation under simulated SOFC interconnect exposure conditions
The IT-SOFC candidate interconnect material ZMG232G10® was thermally pre-treated in air and in H 2 – 3% H 2 O to mitigate dual atmosphere corrosion. Bare and pre-treated steel samples were exposed to a dual atmosphere exposure condition (dry air/metal/4% H 2 – N 2 (bal.) + 3% H 2 O) for 500h at 600°C. Corrosion products and oxide morphology developed on the air-exposed surfaces were analyzed. Pre-treatments of the metal in oxidizing (air) and reducing (H 2 – 3% H 2 O) gas atmospheres provide improved passivation against dual atmosphere corrosion compared to bare steel. Further, the uniform and iron-free oxide scale developed during the pre-treatment of alloy in the low pO 2 H 2 – 3% H 2 O gas atmosphere provides an effective diffusion barrier against the outward transport of cations and oxidation of iron observed under dual atmosphere conditions.