Cross-section SEM-EDS Analysis of Corroded 316 Steel Samples Using JEOL 6610 SEM
Comparison of SEM images obtained for samples 316H-1, 5, 7, and 10 revealed that samples 1 and 5 were subjected to more corrosion than the other two samples. Pores of an average of 1µm size were also observed scattered near the edge of each sample. Corrosion layer thickness was measured from edge of the corroded surface to the pore region. It was found that 316H-1 and 316H-5 had more corrosion damage with 82.40µm and 100µm respectively. Sample 316H-5 posed a challenge in measuring the corrosion layer thickness due to it breaking off from the parent sample during polishing. Samples 316H-7 and 316H-10 are less corroded with 26.57µm and 39.94µm thickness respectively.