Surface characterization of Ti and Ti (6 percent, Al-4 percent, V) metal powders and interaction with primer solutions
The interaction of Ti and Ti 6-4 powders with water and primer solutions was investigated experimentally by measuring the heats of immersion. Similar comparative studies were made on anatase and rutile TiO2 powders. The surface oxide layers of Ti and Ti 6-4 cracked on heating in vacuum between 300 and 400 C as evidenced by high heats of immersion in both water and primer solutions. Polyimide and polyphenylquinoxaline interacted preferentially, compared with the solvents with both metal powders after outgassing at room temperature. The heats of immersion of Ti 6-4 in water, solvents, and primer solutions increased significantly after pretreatment of the powder by an alkaline etch and a phosphate-fluoride process. The TiO2 powders were not satisfactory models for the surface oxide layer on either Ti or Ti 6-4 powder.