Effect of fuel to air ratio on Mach 0.3 burner rig hot corrosion of ZrO2-Y2O3 thermal barrier coatings
A Mach 0.3 burner rig test program was conducted to determine how the fuel to air mass ratio affects the durability of ZrO2-Y2O3/Ni-16Cr-6Al-0.31Y thermal barrier coating systems in combustion products containing 5 ppm Na and 2 ppm V. As the fuel to air mass ratio was increased from 0.039 to 0.049, the durability of ZrO2-6Y2O3, ZrO2-8Y2O3 and ZrO2-12Y2O3 coatings decreased. ZrO2-8Y2O3 coatings were approximately 2X and 1.3X more durable than ZrO2-12Y2O3 and ZrO2-6Y2O3 coatings respectively at the fuel to air mass ratio of 0.039. The number of one hour cycles endured by ZrO2-8Y2O3 coatings varied from averages of 53 to 200 for the fuel to air mass ratios of 0.049 and 0.039, respectively. At the fuel to air mass ratio of 0.049, all ZrO2-Y2O3 coated specimens failed in 40 to 60 one hour cycles