Dependence of depolarization temperature on cation vacancies and lattice distortion for lead-free 74(Bi{sub 1/2}Na{sub 1/2})TiO{sub 3}-20.8(Bi{sub 1/2}K{sub 1/2})TiO{sub 3}-5.2BaTiO{sub 3} ferroelectric ceramics
In this paper, the off-morphotropic-phase-boundary 74(Bi{sub 1/2}Na{sub 1/2})TiO{sub 3}-20.8(Bi{sub 1/2}K{sub 1/2})TiO{sub 3}-5.2BaTiO{sub 3} ceramics were fabricated at different sintering temperatures. It was found out that as the sintering temperature increases, the volatilization of the A-site elements is aggravated, thus generating the oxygen vacancies; meanwhile, the tetragonality of the perovskite lattice reduces gradually. Besides, the temperature-dependent dielectric responses revealed that as the sintering temperature increases, the depolarization temperature T{sub d} decreases while the Curie-Weiss point T{sub C} increases. It is suggested that the lattice distortion, other than the oxygen vacancies, is the crucial factor in influencing the depolarization temperature.