Evaluation of Glovebox Glove Material Integrity Under Thermal Insult (Final Report)
The results of the experiments presented above are summarized in Table 1. Timing of critical events, such as appearance of bubbles on the specimen surface and rupture are noted. Relevant temperature and pressure data are also summarized. These results indicate a few critical aspects of the response of Hypalon glove material when exposed to a high temperature environment. Glove specimens began to show changes in surface appearance (appearance of bubbles on surface) when the temperature at the specimen surface was 530 ± 32 °F, regardless of specimen thickness. The bubbles are likely the result of the glove material decomposing and off-gassing. In the case of the 15 mil thickness gloves, specimens ruptured shortly after bubbling was observed. The ruptures are likely the result the bubbles growing in size, eventually forming pinholes through the thickness of the specimen. It should be noted that the specimens did not need to ignite in order to cause a perforation of the specimen. Specimens located 10, 11 and 12 inches from the burner ruptured, while the specimen located 14 inches from the burner did not rupture; in fact no change in surface appearance was observed. The 30 mil thickness specimens exhibited a different post-bubble response with only the specimen located 10 inches from the burner (i.e. highest surface temperature) resulting in rupture. There was a longer delay between surface bubbling and rupture than was observed in the 15 mil thickness specimens. This specimen also ignited before the specimen ruptured. While the 30 mil thickness specimens located 11 and 12 inches from the burner did show surface bubbling corresponding to thermal breakdown, neither specimen ruptured. Examination of the specimens after testing revealed that a slightly hard layer of melted material had formed on the rear of the specimen. This layer may have acted to seal the rear surface of the specimen by forming a barrier that bubbles could not penetrate. The specimen located 14 inches from the burner did not rupture, and did not exhibit any change in surface characteristics. In general the 30 mil thickness glove materials proved more resistant to thermal-induced rupturing as compared with the 15 mil thickness glove material. It was shown to be possible to rupture a 15 mil thick glove without igniting the glove, while the only test case that resulted in a rupture of a 30 mil thickness specimen also showed the specimen igniting several seconds before eventual rupture. Furthermore, it was observed that 30 mil thickness specimens could be exposed to temperatures high enough to cause decomposition (bubbling), yet not rupture. Thus, it is possible that the 30 mil gloves rupture by burning through the specimen material, while the 15 mil thickness specimens could be ruptured by small bubbles formed by thermal off-gassing expanding and causing pinholes through the specimen thickness. We also note that thermal decomposition and the appearance of surface bubbles was observed in all experiments with a maximum temperature exceeding ∼500 °F. Lastly, we can state that specimens subjected to temperatures below 400 °F experienced no thermal damage, staying below this threshold should prevent damage and potential rupture of either thickness glove materials.